Apr 04, 2022 Zanechajte správu

Extruded aluminum profile surface blister skin, how to deal with?

Bubble or peeling: convex bubbles appear on the surface of the product, common in the head, tail, complete called bubble, has broken called peeling.

Extrusion product bubble, peeling causes

1. The extrusion cylinder and the extrusion pad wear out of tolerance, the size of the extrusion cylinder and the extrusion pad is not properly matched, and the diameter difference of the gasket used exceeds the allowable value;

2. The extrusion cylinder and the extrusion pad are too dirty, with oil, water, graphite, etc.;

3. The lubricating oil contains water;

4. The ingot surface groove is too much, too deep, or the ingot surface has pores, trachoma, loose organization, oil, etc.;

5. The cylinder is not cleaned when the alloy is replaced;

6. Extrusion cylinder temperature and extrusion ingot temperature are too high;

7. The ingot temperature and size exceed the allowed negative deviation;

8. The ingot is too long, the ingot is filled too fast, and the ingot temperature is uneven, resulting in non-drum filling, so the exhaust in the cylinder is incomplete, or improper operation, and the exhaust process is not executed;

9 die hole design is not reasonable, or improper cutting residual material, the residual material in the shunt hole and diversion hole is partly taken out, and the gas in the gap enters the surface when extrusion.

The method of eliminating bubbles and peeling of extruded products

1. Reasonably design the matching size of the extrusion cylinder and the extrusion gasket, check the size of the tool frequently to ensure that it meets the requirements, repair the extrusion cylinder in time when there is a big belly, and the extrusion gasket can not exceed the tolerance;

2. Keep the surface of tools and ingot clean, smooth and dry;

3. When replacing the alloy, clean the cylinder thoroughly;

4. Check the equipment and instruments regularly to prevent the temperature from being too high and the speed too fast;

5. Strictly implement the process procedures and systems;

6. Design and manufacture molds reasonably, with 1 degree -3 degree internal slope for diversion holes and diversion holes;

7. Strict operation, correct shear residual material and complete exhaust.


Zaslať požiadavku